The most common high-strength metric bolt grade. Minimum tensile 800 MPa (d ≤ 16) / 830 MPa (d > 16); quenched and tempered carbon steel, boron-added steel and alloy steel.
Key points
- Nominal tensile 800 MPa × yield ratio 0.8 = nominal yield 640 MPa.
- d ≤ 16 mm: minimum tensile 800, 0.2 % proof strength 640, proof stress 580 MPa, 250–320 HV (22–32 HRC).
- d > 16 mm: minimum tensile 830, 0.2 % proof strength 660, proof stress 600 MPa, 255–335 HV (23–34 HRC).
- Minimum elongation 12 %; for d ≥ 16 mm, impact at −20 °C of 27 J or more.
- Material: carbon steel with boron etc. added, carbon steel, alloy steel, quenched and tempered (tempering 425 °C or higher).
- Mating: nut class 8 (ISO 898-2), washer 200HV (ISO 898-3).
- A grade that does not need baking when electroplated (below 10.9, ISO 4042), and it is eligible for hot-dip galvanizing (ISO 10684).
Checks for BOMs and buying
- 8.8 ≈ F3125 A325 (minimum 120 ksi) is an approximate correspondence. A449 is about 25 % lower than 8.8 (830 MPa) at minimum 90 ksi (about 621 MPa, converted) for 1-3/4" and above, so do not treat them as corresponding.
- The judgment values differ at the 16 mm diameter boundary. M16 is judged by the d ≤ 16 values.
- If class 5 or 6 nuts are used with 8.8 bolts, the nut threads may strip first.
- The hardness range (22–34 HRC) exceeds the sour service limit (22 HRC or below), so it is not used for H2S-exposed bolting.
- The structural HR 8.8 set (EN 14399-3) has set requirements different from an ordinary 8.8 hexagon bolt.
These links go to the issuing bodies; they are not the verification source of individual values.
Basis: ISO 898-1 · ISO 898-2 · ISO 898-3 · ISO 4042 · library-wide review 2026-10 (no per-item review date). Project edition, tolerances and service conditions must be confirmed against the standard text and supplier documents. Do not estimate unconfirmed values.