A procedure that measures the alloy composition of a part with an on-site analyzer to confirm that the specified material is correct. It only distinguishes the material family by alloying elements and does not tell heat treatment, hardness, or strength.
Key points
- Handheld XRF quickly measures alloying elements such as Cr · Ni · Mo · V but cannot measure light elements such as carbon.
- Spark OES can measure up to carbon but grinds the surface and leaves discharge marks, so choose a measurement position that is not the threaded portion or bearing face.
- B7 and B7M are usually made of the same family of steel (4140, etc.) and are distinguished by heat treatment and hardness, so they are not distinguished even by an analysis that measures carbon. Confirm by hardness results and markings.
- 304 and 316 (A2 · A4 series) are distinguished by Mo. Materials that differ only in carbon content, such as 304 and 304L, and 316 and 316L, cannot be distinguished by XRF.
- Material verification programs for refinery and petrochemical facilities often refer to API RP 578.
- A PMI result is only a confirmation of the material family and does not replace an EN 10204 certificate.
What PMI can and cannot distinguish
| Comparison | Handheld XRF | Confirmation method |
|---|---|---|
| B8 ↔ B8M (usually 304 ↔ 316) | Yes (Mo) | Composition + marking |
| A2 ↔ A4 | Yes (Mo) | Composition + marking |
| 304 ↔ 304L, 316 ↔ 316L | No (only C differs) | Analysis that measures carbon (OES, etc.), certificate |
| B7 ↔ B7M | No (usually the same family of steel) | Hardness results, marking |
| 8.8 ↔ 10.9 | No (material ranges overlap, the grade is decided by heat treatment) | Marking, hardness · tensile |
XRF = handheld X-ray fluorescence analyzer. The measurable elements differ by instrument, so check the measured elements on the result sheet.
Checks for BOMs and buying
- A "PMI done" mark is meaningful only if there is a record of who measured which part with what equipment. Require the equipment type, measured elements, and acceptance criteria on the result sheet.
- The claim that B7M was confirmed by PMI does not hold. Confirm B7M by hardness test records and markings.
- It is normal for an XRF result to have no carbon. If confirmation of L grades (low carbon) is needed, specify a method that can measure carbon.
ASTM: official search ↗ · ISO: official search ↗ · API: official search ↗
These links go to the issuing bodies; they are not the verification source of individual values.
Basis: API RP 578 · ASTM A193/A193M · ISO 3506-1 · ISO 898-1 · library-wide review 2026-10 (no per-item review date). Project edition, tolerances and service conditions must be confirmed against the standard text and supplier documents. Do not estimate unconfirmed values.